Metallographic Etchants - Carbon Steels

Metallographic Etchants

High Carbon Steel Etchants

CAUTION: Safety is very important when etching. Be sure to wear the appropriate protective clothing and observe all WARNINGS on chemical manufacturers MSDS. Also review COMMENTS Section for each etchant.

Etchant

Conc.

Conditions

Comments

Picral
Ethanol
Picric acid

100 ml
2-4 grams

Seconds to minutes

For heat treated steels

Do not let etchant dry – explosive

Ethanol
Nitric acid
Hydrochloric acid
Picric acid

80 ml
10 ml
10 ml
1 gram

Seconds to minutes

Grain boundaries

Nital
Ethanol
Nitric acid

100 ml
1-10 ml

Seconds to minutes

Do not exceed 10% nitric acid -explosive


Metallographic micrograph of high carbon steel
1095 High Carbon Steel (furnace cooled), etched, Mag. 100X

About Us | Site Map | Disclaimer and Legal Information | Contact Us

Copyright © 2006
Pace Technologies - 1802 W. Grant Rd. No. 102 - Tucson, AZ 85745 USA
Telephone 520-882-6598 FAX 520-882-6599.
All Rights Reserved.