Metallographic Etchants - Tin

Metallographic Etchants

Tin Alloy Etchants

CAUTION: Safety is very important when etching. Be sure to wear the appropriate protective clothing and observe all WARNINGS on chemical manufacturers MSDS. Also review COMMENTS Section for each etchant.

Etchant

Conc.

Conditions

Comments

Ethanol or methanol
or Distilled water
Hydrochloric acid


100 ml
2-5 ml

Several minutes

Pure tin, tin-lead alloys, tin-antimony-copper alloys

Nital
Ethanol
Nitric acid


100 ml
1-10 ml

Seconds to minutes

Do not exceed 10% nitric acid -explosive

Distilled water or methanol
Hydrochloric acid
Ferric chloride

100 ml
5-25 ml
10 grams

Seconds to minutes

Tin-copper alloys


Metallographic micrograph of etched tin-copper alloy
Tin-copper alloy, etched with 2% Nital, Mag. 100X (DIC)

About Us | Site Map | Disclaimer and Legal Information | Contact Us

Copyright © 2006
Pace Technologies - 1802 W. Grant Rd. No. 102 - Tucson, AZ 85745 USA
Telephone 520-882-6598 FAX 520-882-6599.
All Rights Reserved.