Manganese Aluminum Bronze Specimen Preparation
(Class 1 Procedures)

Metallographic Class 1 sample preparation


Manganese-aluminum bronze is a relatively harder bronze because of the addition of manganese. Microstructural preparation of this material is relatively straight forward.

SECTIONING

MAXCUT Abrasive blade (MAX-C or MAX-I series)

MOUNTING

Compression Mounting with Phenolic, Epoxy or Diallyl Phthalate compression mounting resins

POLISHING

Abrasive/surface

Lubricant

Force/ sample

Speed
(Head/base)

Time

Individual
Force mode

Central Force
mode

120 grit SiC paper
240 grit SiC paper

Water

5-10 lbs

200/200 rpm

Until plane
1 minute

 

360 grit SiC paper
600 grit SiC paper
800 grit SiC paper
1200 grit SiC paper

Water

5-10 lbs

200/200 rpm

1 minute
1 minute
1 minute
1 minute

Metallographic individual polishing force

6 um DIAMAT diamond on TEXPAN polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

2 minutes

Metallographic individual polishing force

1 um DIAMAT diamond on GOLDPAD or ATLANTIS polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

2 minutes

Metallographic individual polishing force

0.05 um Nanometer alumina on NAPPAD polishing pad

 

5-10 lbs

100/100 rpm

1 minute

Metallographic individual polishing force

*Required for central polishing force. Click here for more information on central vs. individual polishing force polishing.

Metallographic micrograph of Nickel Iron Bronze

Mangnese-Aluminum Bronze, 400X DIC (etchant: ammonium persulface, HCl, DI Water)


Return to top

PACE TECHNOLOGIES CONTACT


PACE Technologies
3601 E. 34th St.
Tucson, Arizona 85713
+1-520-882-6598
FAX +1-520-882-6599
email: pace@metallographic.com
www.metallographic.com


Information Requests

*Required Information

*Company:
*Name:
*E-mail:
Title:
*Address:
P.O. / Suite:
*City:
*State:
*Zip Code:
Country:
*Phone:
Fax:

Industry:

Process Type:

Send Equipment Quotes
Add my name to PACE Technologies mailing list
Send NEW 2018-2020 Product catalog
Send me my FREE MET MANUAL
Request a salesperson call


Metallographic
Consumables

Brochures:

For online
ordering
click here
Online Ordering
Abrasive Blades
Diamond Blades
Compression Mounting
Castable Mounting
Polishing Pads
Lapping Films
Diamond Disks
Composite Disks
Polycrystalline Diamond
Monocrystalline Diamond
Final Polishing Abrasives
Etchants
Consumables Catalog



Metallographic
Equipment

Brochures:

For specific
equipment quotes
click here
Quotes
Abrasive Cutters
Precision Wafering Saws
Compression Mounting Presses
Castable Vacuum Chamber
Manual Roll and Belt Grinders
Polishing Machines
Automated Polishing Heads
Vibratory Polisher



Metallographic
Analysis
Brochures:

For specific
instrument quotes
click here
Quotes

Microscopes
Microhardness Testers
Rockwell Hardness Testers
Brinell Hardness Testers
MacroVickers Hardness Tester
Image Analysis



Laboratory
Furniture
Brochures:

For specific
items quotes
click here
Quotes

Lab Benches
Microscope Benches
Fume Hood
Safety Cabinets
Specimen Storage Cabinet

Other Questions

Question To:
Enter Request Info. or Question:

Return to top


About Us | Site Map | Web Disclaimer | Terms and Conditions | Contact Us

Copyright 2006-2018
PACE Technologies ® - 3601 E. 34th St., Tucson, AZ 85713, USA
Telephone +1 520-882-6598 FAX +1 520-882-6599
All Rights Reserved


PACE Technologies facebook link Blog us on Tumblr Blog us on Tumblr PACE Technologies Google+ PACE Technologies Google+ PACE Technologies Google+