Tool Steel Specimen Preparation
(Class 8 Procedures)

Metallographic Class 8 sample preparation


Tool steels are very hard steels, typically in the range of Rc 50-60. Microstructural preparation is relatively staight forward. With the use of polycrystalline diamond and nanometer alumina abrasives, these very hard materials can be very easy to polish.

SECTIONING

MAXCUT Abrasive blade (Cat. No. MAX-E or MAX-V series)

MOUNTING

Compression Mounting with Phenolic, Epoxy or Diallyl Phthalate compression mounting resins

POLISHING

Abrasive/surface

Lubricant

Force/ sample

Speed
(Head/base)

Time

Individual
Force mode

Central Force
mode

120 grit SiC paper*
240 grit SiC paper*

Water

5-10 lbs

200/200 rpm

Until plane
1 minute

 

360 grit SiC paper
600 grit SiC paper

Water

5-10 lbs

200/200 rpm

1 minute
1 minute

Metallographic individual polishing force

9 um DIAMAT diamond on POLYPAD polishing pad

DIALUBE Purple Extender

5 lbs

200/200 rpm

3 minutes

Metallographic individual polishing force

3 um DIAMAT diamond on TEXPAN polishing pad

DIALUBE Purple Extender

5 lbs

200/200 rpm

3 minutes

Metallographic individual polishing force

1 um DIAMAT diamond on GOLDPAD polishing pad

DIALUBE Purple Extender

5-10 lbs

200/200 rpm

2 minutes

Metallographic individual polishing force

0.05 um Nanometer alumina on MICROPAD polishing pad

 

5 lbs

100/100 rpm

30 seconds

Metallographic individual polishing force

*Required for central polishing force. Click here for more information on central vs. individual polishing force polishing.

Metallographic micrograph of manganese vanadium tool steel

44 MnV F6 Steel, 500X, 3 second nital etch

High alloy tool steel micrograph

High alloy tool steel, 200X (BF), Etchant Picral

ETCHING

Common Etchants
PACE Technologies Recommended Etchants

PACE Technologies Etchant Database

CAUTION:Safety is very important when etching. Be sure to wear the appropriate protective clothing and observe all WARNINGS on chemical manufacuters SDS (Safety Data Sheets). Also review the COMMENTS and CONDITIONS Section for each etchant.


Return to top

PACE TECHNOLOGIES CONTACT


PACE Technologies
3601 E. 34th St.
Tucson, Arizona 85713
+1-520-882-6598
FAX +1-520-882-6599
email: pace@metallographic.com
www.metallographic.com


Information Requests

*Required Information

*Company:
*Name:
*E-mail:
Title:
*Address:
P.O. / Suite:
*City:
*State:
*Zip Code:
Country:
*Phone:
Fax:

Industry:

Process Type:

Send Equipment Quotes
Add my name to PACE Technologies mailing list
Send NEW 2018-2020 Product catalog
Send me my FREE MET MANUAL
Request a salesperson call


Metallographic
Consumables

Brochures:

For online
ordering
click here
Online Ordering
Abrasive Blades
Diamond Blades
Compression Mounting
Castable Mounting
Polishing Pads
Lapping Films
Diamond Disks
Composite Disks
Polycrystalline Diamond
Monocrystalline Diamond
Final Polishing Abrasives
Etchants
Consumables Catalog



Metallographic
Equipment

Brochures:

For specific
equipment quotes
click here
Quotes
Abrasive Cutters
Precision Wafering Saws
Compression Mounting Presses
Castable Vacuum Chamber
Manual Roll and Belt Grinders
Polishing Machines
Automated Polishing Heads
Vibratory Polisher



Metallographic
Analysis
Brochures:

For specific
instrument quotes
click here
Quotes

Microscopes
Microhardness Testers
Rockwell Hardness Testers
Brinell Hardness Testers
MacroVickers Hardness Tester
Image Analysis



Laboratory
Furniture
Brochures:

For specific
items quotes
click here
Quotes

Lab Benches
Microscope Benches
Fume Hood
Safety Cabinets
Specimen Storage Cabinet

Other Questions

Question To:
Enter Request Info. or Question:

Return to top


About Us | Site Map | Web Disclaimer | Terms and Conditions | Contact Us

Copyright 2006-2019
PACE Technologies ® - 3601 E. 34th St., Tucson, AZ 85713, USA
Telephone +1-520-882-6598 FAX +1-520-882-6599
All Rights Reserved


PACE Technologies facebook link Blog us on Tumblr Blog us on Tumblr PACE Technologies Google+ PACE Technologies Google+ PACE Technologies Google+