Inconel

Corrosion resistant materials such as Inconnel are relatively easy to polish by standard metallographic techniques. However, the results can be significantly improved by using finely graded nanometer alpha alumina polishing solutions.

SECTIONING

MAXCUT Abrasive blade (Cat. No. MAX-D or MAX-I series)

MOUNTING
Compression Mounting with Phenolic, Epoxy or Diallyl Phthalate compression mounting resins

POLISHING

Abrasive/surface

Lubricant

Force/ sample

Time

240 grit SiC paper
320 grit SiC paper
400 grit SiC paper
600 grit SiC paper

Water
Water
Water
Water

5 lbs
5 lbs
5 lbs
5 lbs

Until plane
1 minute
1 minute
1 minute

9 um DIAMAT diamond on POLYPAD polishing pad

DIALUBE Purple Extender

5 lbs

2 minutes

6 um DIAMAT diamond on TEXPAN polsihing pad

DIALUBE Purple Extender

5 lbs

2 minutes

1 um DIAMAT diamond on GOLDPAD polishing pad

DIALUBE Purple Extender

5 lbs

2 minutes

0.05 um Nanometer alumina on NAPPAD polishing pad

 

5 lbs

30 seconds


About Us | Site Map | Disclaimer and Legal Information | Contact Us

Copyright © 2011
PACE Technologies - 3601 E. 34th St. - Tucson, AZ 85713 USA
Telephone +1 520-882-6598 FAX +1 520-882-6599.
All Rights Reserved.