Na₂S₂O₅ 10%Sodium Metabisulfite
Sodium Metabisulfite (10%)
Specialty
Composition
10g Na₂S₂O₅, 100ml H₂O
10%
Method
Immersion
Time
30s
Alternative Names
Tags
Reveals
Prior austenite grain boundaries
Typical Results
For revealing prior austenite grain boundaries in quenched and tempered steels. Important for heat treatment analysis.
Color Effects
Prior austenite boundaries dark
Compatible Materials
Incompatible Materials
Application Method
Method:immersion
Typical Time:30 seconds
Preparation Notes
Dissolve 10g sodium metabisulfite (Na₂S₂O₅) in 100ml distilled water. Prepare fresh solution.
Application Notes
Immerse sample for 30-60 seconds. Swab gently if needed. Rinse with water.
Troubleshooting
Prepare fresh for best results. Solution decomposes over time. Important for heat treatment analysis.
Storage Notes
Store in dark bottle. Prepare fresh when needed. Shelf life: 1-2 days.
Alternative Etchants
- 2% Nital
- 3% Nital
Similar Etchants
- 2% Nital