Incoloy 925

Nickel Alloy

Basic Information

Category: Nickel Alloy
Material Type: alloy
Alternative Names:
Incoloy 925UNS N09925Alloy 925
Tags:
precipitation-hardeningcorrosion-resistantnickel-iron

Composition & Structure

Composition: Ni-21Cr-30Fe-3Mo-2.3Cu-0.9Ti-0.6Al
Microstructure: Austenite with gamma prime precipitates

Description

Precipitation-hardening nickel-iron alloy with excellent strength and corrosion resistance. Used in demanding oil and gas applications.

Mechanical Properties

Hardness: 310 HB
Hardness (HB): 310 HB
Hardness (HRC): 32 HRC
Hardness Category: very hard
Tensile Strength: 860 MPa
Yield Strength: 690 MPa

Physical Properties

Density: 8.14 g/cm³
Melting Point: 1377 °C

Material Characteristics

Work Hardening: No
Magnetic: No
Corrosion Resistance: excellent

Sectioning

Use slow-speed diamond saw or abrasive cut-off wheel designed for non-ferrous materials. Standard cut-off wheel (1.0-1.5 mm thickness) is appropriate. Use adequate coolant flow to prevent overheating and minimize deformation. Cutting speed: 150-250 RPM for most cut-off saws. Apply steady, moderate pressure - the material allows for reasonable feed rates. Avoid forcing the cut which can cause wheel wear and sample damage. Leave adequate allowance (~2-3 mm) for grinding away the heat-affected zone from cutting.

Mounting

Cold mounting with epoxy resin is preferred to avoid heat that could affect the microstructure. Use a low-shrinkage epoxy resin for best edge retention. Ensure complete cure before grinding to prevent edge rounding and maintain sample integrity.

Hot compression mounting is acceptable if the part tolerates ~150-180°C and moderate pressure (2000-3000 psi for phenolic). Use phenolic or epoxy-phenolic resins. Ensure proper cooling under pressure to minimize shrinkage.

Grinding

The hardness (310 HB) of Incoloy 925 requires careful grinding. Use standard SiC grinding papers with adequate water lubrication. Disc speed: 200-300 RPM. Apply light to moderate pressure (30-40 N per 30 mm sample) - the hard material may require longer grinding times. Use sharp, fresh grinding papers to minimize deformation.

Grinding sequence:
  • 120 grit: Remove sectioning damage (40-90 seconds). Use moderate pressure to remove heat-affected zone.
  • 240 grit: Remove previous scratches (40-90 seconds). Ensure complete scratch removal.
  • 320 grit: Remove previous scratches (40-90 seconds). Ensure complete scratch removal.
  • 400 grit: Remove previous scratches (40-90 seconds). Ensure complete scratch removal.
  • 600 grit: Remove previous scratches (40-90 seconds). Ensure complete scratch removal.
Always rotate the specimen holder 90° between steps to ensure complete scratch removal. Use complementary rotation (platen and holder same direction, different speeds) rather than contra-rotation to minimize deformation. Adequate water lubrication is critical - avoid drying during grinding which can cause smearing.
Recommended Sequence:
120240320400600

Polishing

The hardness requires careful polishing. Use diamond polishing with appropriate polishing pads for each stage. Apply light to moderate pressure throughout to prevent deformation.

Diamond polishing sequence:
  • 9μm diamond: 2-4 minutes on a medium-hard synthetic pad (e.g., TEXPAN) with light to moderate pressure (30-40 N per 30 mm sample). Start with 9μm to minimize damage. The hard material may require longer polishing times.
  • 3μm diamond: 2-4 minutes on a medium-hard synthetic pad (e.g., TEXPAN) with light pressure (25-35 N). Continue removing scratches from previous step.
  • 1μm diamond: 2-3 minutes on a medium-hard synthetic pad with lighter pressure (25-35 N). These pads provide gentle material removal.
  • 0.05μm colloidal silica: 1-2 minutes on a high-napped final polishing pad (e.g., MICROPAD) with very light pressure. This removes any remaining fine scratches and prepares the surface for etching. Monitor for relief - reduce polishing time if excessive relief develops.
Use appropriate polishing lubricants. The hard material means polishing times should be sufficient but not excessive - avoid over-polishing which can cause relief and affect grain boundary revelation. Monitor the surface frequently under the microscope to check for smearing or excessive relief.
Recommended Sequence:
9μm diamond3μm diamond1μm diamond0.05μm colloidal silica

Etching

Incoloy 925 responds well to standard etchants for nickel alloy materials. The austenite with gamma prime precipitates will reveal clearly with appropriate etchants. Glyceregia (Chemical Etching) - Primary choice for general microstructure:
  • Composition: 10ml glycerol, 15ml HCl, 5ml HNO₃
  • Preparation: Add acids to glycerol slowly with stirring. Prepare fresh for best results. The glycerol moderates the reaction rate.
  • Application: Immerse sample or swab for 10-30 seconds. Classic general-purpose micro-etchant for austenitic stainless steels and nickel alloys.
  • Reveals: Grain boundaries, grain structure, and twin boundaries clearly. Excellent for general microstructure examination.
  • Rinse: Immediately with water, then ethanol. Dry with compressed air or warm air to avoid staining.
  • Note: Prepare fresh when needed. Shelf life: several hours. Use in fume hood.
Electrolytic 10% Oxalic (Chemical Etching) - Standard etchant for this material:
  • Application: Follow standard procedures for Electrolytic 10% Oxalic.
  • Reveals: Grain boundaries and microstructure clearly.
  • Rinse: Immediately with water, then ethanol. Dry with compressed air.
  • Note: Use appropriate safety measures. Consult material-specific guidelines.
Etching Strategy:
  • Start with Glyceregia for general microstructure examination
  • Always clean and degrease before etching
  • Use short initial etch times (a few seconds), check under the microscope, repeat if needed
  • Check etching progress frequently - over-etching can obscure fine details
Safety: All etchants require proper PPE (gloves, safety glasses, lab coat), proper fume hood, and appropriate safety measures. Handle with care.
Common Etchants:
GlyceregiaElectrolytic 10% Oxalic

Heat Treatment

Solution treated and aged

Temperature Parameters

Annealing Temperature: 1150 °C

No standards information available.

Applications

  • Oil and gas
  • Chemical processing
  • Marine

Typical Uses

  • Oil and gas equipment
  • Chemical reactors
  • Marine equipment