Skip to main content

O1 Oil-Hardening Tool Steel

Tool Steel

Basic Information

Category: Tool Steel
Material Type: alloy
Alternative Names:
O1AISI O11.2510
Tags:
cold-workoil-hardeninggeneral-purpose

Composition & Structure

Composition: Fe-0.90C-1.0Mn-0.5Cr-0.5W
Microstructure: Tempered martensite

Description

Oil-hardening tool steel with good machinability. General-purpose tool steel for cold-work applications.

Mechanical Properties

Hardness: 217 HB
Hardness (HB): 217 HB
Hardness Category: medium
Tensile Strength: 760 MPa
Yield Strength: 620 MPa

Physical Properties

Density: 7.81 g/cm³
Melting Point: 1420 °C

Material Characteristics

Work Hardening: No
Magnetic: Yes
Corrosion Resistance: low

Sectioning

Use abrasive cut-off wheel designed for steel (Al₂O₃ or SiC abrasive). Standard cut-off wheel (1.0-1.5 mm thickness) is appropriate. Use adequate coolant flow to prevent overheating - excessive heat can affect the microstructure. Cutting speed: 200-300 RPM for most cut-off saws. Apply steady, moderate pressure - the material allows for reasonable feed rates. Avoid forcing the cut which can cause wheel wear and sample damage. Leave adequate allowance (~2-3 mm) for grinding away the heat-affected zone from cutting.

Mounting

Cold mounting with epoxy resin is preferred to avoid heat that could affect the microstructure. Use a low-shrinkage epoxy resin for best edge retention. Ensure complete cure before grinding to prevent edge rounding and maintain sample integrity.

Hot compression mounting is acceptable if the part tolerates ~150-180°C and moderate pressure (2000-3000 psi for phenolic). Use phenolic or epoxy-phenolic resins. Ensure proper cooling under pressure to minimize shrinkage.

Grinding

The medium hardness (217 HB) of O1 Oil-Hardening Tool Steel requires careful grinding. Use standard SiC grinding papers with adequate water lubrication. Disc speed: 200-300 RPM. Apply light to moderate pressure (25-35 N per 30 mm sample) - avoid excessive force that could cause work hardening. Use sharp, fresh grinding papers to minimize deformation.

Grinding sequence:
  • 120 grit: Remove sectioning damage (30-60 seconds). Use moderate pressure to remove heat-affected zone.
  • 240 grit: Remove previous scratches (30-60 seconds). Ensure complete scratch removal.
  • 320 grit: Remove previous scratches (30-60 seconds). Ensure complete scratch removal.
  • 400 grit: Remove previous scratches (30-60 seconds). Ensure complete scratch removal.
  • 600 grit: Remove previous scratches (30-60 seconds). Ensure complete scratch removal.
Always rotate the specimen holder 90° between steps to ensure complete scratch removal. Use complementary rotation (platen and holder same direction, different speeds) rather than contra-rotation to minimize deformation. Adequate water lubrication is critical - avoid drying during grinding which can cause smearing.
Recommended Sequence:
120240320400600

Polishing

The medium hardness requires careful polishing. Use diamond polishing with appropriate polishing pads for each stage. Apply light to moderate pressure throughout to prevent deformation.

Diamond polishing sequence:
  • 9μm diamond: 2-4 minutes on a medium-hard synthetic pad (e.g., TEXPAN) with light to moderate pressure (25-35 N per 30 mm sample). Start with 9μm to minimize damage. ensure complete scratch removal at each step.
  • 3μm diamond: 2-4 minutes on a medium-hard synthetic pad (e.g., TEXPAN) with light pressure (20-30 N). Continue removing scratches from previous step.
  • 1μm diamond: 2-3 minutes on a medium-hard synthetic pad with lighter pressure (20-30 N). These pads provide gentle material removal.
  • 0.05μm colloidal silica: 1-2 minutes on a high-napped final polishing pad (e.g., MICROPAD) with very light pressure. This removes any remaining fine scratches and prepares the surface for etching. Monitor for relief - reduce polishing time if excessive relief develops.
Use appropriate polishing lubricants. The medium material means polishing times should be sufficient but not excessive - avoid over-polishing which can cause relief and affect grain boundary revelation. Monitor the surface frequently under the microscope to check for smearing or excessive relief.
Recommended Sequence:
9μm diamond3μm diamond1μm diamond0.05μm colloidal silica

Etching

O1 Oil-Hardening Tool Steel responds well to standard etchants for tool steel materials. The tempered martensite will reveal clearly with appropriate etchants. 2% Nital (Chemical Etching) - Primary choice for carbon steels:
  • Composition: 2ml HNO₃ (concentrated), 98ml ethanol
  • Preparation: Add nitric acid to ethanol slowly with stirring. Prepare fresh for best results. Solution is stable for several days if stored properly.
  • Application: Immerse sample or swab for 5-15 seconds. Standard etchant for carbon steels.
  • Reveals: Ferrite grain boundaries and pearlite structure clearly. Excellent for general microstructure examination.
  • Rinse: Immediately with water, then ethanol. Dry with compressed air or warm air to avoid staining.
  • Note: Prepare fresh when needed. Shelf life: several days. Use in fume hood.
4% Picral (Chemical Etching) - For revealing pearlite structure:
  • Composition: 4g picric acid, 100ml ethanol
  • Preparation: Dissolve picric acid in ethanol with stirring. Prepare fresh for best results. Solution is stable for several weeks if stored properly.
  • Application: Immerse sample or swab for 10-60 seconds. Excellent for revealing pearlite structure without attacking ferrite boundaries.
  • Reveals: Pearlite structure clearly with excellent contrast. Less aggressive on ferrite grain boundaries than nital.
  • Rinse: Immediately with water, then ethanol. Dry with compressed air.
  • Note: Prepare fresh when needed. Shelf life: several weeks if stored properly. Use in fume hood. Picric acid is explosive when dry - keep moist and handle with care.
Etching Strategy:
  • Start with 2% Nital for general microstructure examination
  • Always clean and degrease before etching
  • Use short initial etch times (a few seconds), check under the microscope, repeat if needed
  • Check etching progress frequently - over-etching can obscure fine details
Safety: All etchants require proper PPE (gloves, safety glasses, lab coat), proper fume hood, and appropriate safety measures. Handle with care.
Common Etchants:
2% Nital4% Picral

Heat Treatment

Oil quenched and tempered

Temperature Parameters

Annealing Temperature: 790 °C

No standards information available.

Applications

  • Cutting tools
  • Dies
  • Gauges

Typical Uses

  • Cutting tools
  • Punches
  • Gauges