| Etchant | Conc. | Conditions | Comments |
|---|---|---|---|
|
Ethanol or methanol or Distilled water Hydrochloric acid |
100 ml 2-5 ml |
Several minutes | Pure tin, tin-lead alloys, tin-antimony-copper alloys |
|
Nital: Ethanol Nitric acid |
100 ml 1-10 ml |
Seconds to minutes |
Do not exceed 10% nitric acid -explosive |
|
Distilled water or methanol
Hydrochloric acid Ferric chloride |
100 ml 5-25 ml 10 gm |
Seconds to minutes |
Tin-copper alloys |
![]() |
| Tin-copper alloy, etched with 2% Nital, Mag. 100X (DIC) |