2024 Aluminum Alloy Specimen Preparation
(Class 1 Procedures)

Metallographic Class 1 sample preparation


The difficulty in preparing these materials arises from the fact that these materials have oxide inclusions in the microstructure. Proper specimen preparation retains these oxides and thus eliminates scratching and smearing from these particles. If the specimen is not prepared properly, the microstructure will not be accurately represented.

SECTIONING

MAXCUT Abrasive blade (Cat. No. MAX-C or MAX-I series)

MOUNTING

Compression Mounting with Phenolic, Epoxy or Diallyl Phthalate compression mounting resins

POLISHING

Abrasive/surface

Lubricant

Force/ sample

Speed
(Head/base)

Time

P220 grit ALO paper
P500 grit ALO paper
P1200 grit ALO paper

Water

5-10 lbs

100/100 rpm

Until plane
1 minute
1 minute

1 um DIAMAT diamond on ATLANTIS polishing pad

DIALUBE Purple Extender

5-10 lbs

100/100 rpm

2 minutes

0.05 um Nanometer alumina on NAPPAD polishing pad

 

5-10 lbs

100/100 rpm

1 minute


Metallographic micrograph of 2024 aluminum alloy

2024 Aluminum Alloy, Etched Kellers Reagent, 200X

ETCHING

Common Etchants
PACE Technologies Recommended Etchants

PACE Technologies Etchant Database

CAUTION:Safety is very important when etching. Be sure to wear the appropriate protective clothing and observe all WARNINGS on chemical manufacuters SDS (Safety Data Sheets). Also review the COMMENTS and CONDITIONS Section for each etchant.


Return to top

PACE TECHNOLOGIES CONTACT


PACE Technologies
3601 E. 34th St.
Tucson, Arizona 85713
+1-520-882-6598
FAX +1-520-882-6599
email: pace@metallographic.com
www.metallographic.com


Information Requests

*Required Information

*Company:
*Name:
*E-mail:
Title:
*Address:
P.O. / Suite:
*City:
*State:
*Zip Code:
Country:
*Phone:
Fax:

Industry:

Process Type:

Send Equipment Quotes
Add my name to PACE Technologies mailing list
Send Product catalog
Send me my FREE MET MANUAL
Request a salesperson call
Add me to Newsletter Distribution


Metallographic
Consumables

Brochures:

For online
ordering
click here
Online Ordering
Abrasive Blades
Diamond Blades
Compression Mounting
Castable Mounting
Polishing Pads
Lapping Films
Diamond Disks
Composite Disks
Polycrystalline Diamond
Monocrystalline Diamond
Final Polishing Abrasives
Etchants
Consumables Catalog



Metallographic
Equipment

Brochures:

For specific
equipment quotes
click here
Quotes
Abrasive Cutters
Precision Wafering Saws
Compression Mounting Presses
Castable Vacuum Chamber
Manual Roll and Belt Grinders
Polishing Machines
Automated Polishing Heads
Vibratory Polisher



Metallographic
Analysis
Brochures:

For specific
instrument quotes
click here
Quotes

Microscopes
Microhardness Testers
Rockwell Hardness Testers
Brinell Hardness Testers
MacroVickers Hardness Tester
Image Analysis



Laboratory
Furniture
Brochures:

For specific
items quotes
click here
Quotes

Lab Benches
Microscope Benches
Fume Hood
Safety Cabinets
Specimen Storage Cabinet

Other Questions

Question To:
Enter Request Info. or Question:

Return to top


About Us | Site Map | Web Disclaimer | Terms and Conditions | Contact Us

Copyright 2006-2018
PACE Technologies ® - 3601 E. 34th St., Tucson, AZ 85713, USA
Telephone +1 520-882-6598 FAX +1 520-882-6599
All Rights Reserved


PACE Technologies facebook link Blog us on Tumblr Blog us on Tumblr PACE Technologies Google+ PACE Technologies Google+ PACE Technologies Google+