120 grit SiC paper*
240 grit SiC paper*
|
Water |
5-10 lbs |
200/200 rpm |
Planar
1 min
|
|
 |
360 grit SiC paper
600 grit SiC paper
|
Water |
5-10 lbs |
200/200 rpm |
1 min
1 min |
 |
 |
9 um DIAMAT diamond
on POLYPAD polishing pad |
DIALUBE Purple
Extender |
5 lbs |
200/200 rpm |
3 min |
 |
 |
6 um DIAMAT diamond
on TEXPAN polishing pad |
DIALUBE Purple
Extender |
5 lbs |
200/200 rpm |
3 min |
 |
 |
1 um DIAMAT diamond
on GOLDPAD polishing pad |
DIALUBE Purple
Extender |
5-10 lbs |
200/200 rpm |
2 min |
 |
 |
Titanium Attack mixed
with Kroll's reagent on
MICROPAD polishing pad |
|
5-10 lbs |
200/200 rpm |
5-10 min |
 |
 |